利用報告書 / User's Reports

  • 印刷する

【公開日:2024.07.25】【最終更新日:2025.03.14】

課題データ / Project Data

課題番号 / Project Issue Number

23UT1106

利用課題名 / Title

Characterization of the out-of-plane deformation of shear band on metal surface

利用した実施機関 / Support Institute

東京大学 / Tokyo Univ.

機関外・機関内の利用 / External or Internal Use

内部利用(ARIM事業参画者以外)/Internal Use (by non ARIM members)

技術領域 / Technology Area

【横断技術領域 / Cross-Technology Area】(主 / Main)計測・分析/Advanced Characterization(副 / Sub)-

【重要技術領域 / Important Technology Area】(主 / Main)その他/Others(副 / Sub)-

キーワード / Keywords

Titanium-based alloys, out-of-plane deformation, a dwell-fatigue loading,光学顕微鏡/ Optical microscope


利用者と利用形態 / User and Support Type

利用者名(課題申請者)/ User Name (Project Applicant)

榎 学

所属名 / Affiliation

東京大学工学系研究科マテリアル工学専攻

共同利用者氏名 / Names of Collaborators in Other Institutes Than Hub and Spoke Institutes
ARIM実施機関支援担当者 / Names of Collaborators in The Hub and Spoke Institutes
利用形態 / Support Type

(主 / Main)機器利用/Equipment Utilization(副 / Sub)-


利用した主な設備 / Equipment Used in This Project

UT-850:形状・膜厚・電気特性評価装置群


報告書データ / Report

概要(目的・用途・実施内容)/ Abstract (Aim, Use Applications and Contents)

To characterize the out-of-plane deformation along slip bands of a titanium-based alloy under dwell-fatigue conditions.

実験 / Experimental

A tensile specimen was subjected to a dwell-fatigue loading (peak stress: 870 MPa, r ratio: 0.1) to1000 cycles. Out of plane deformation of the specimen surface was characterized by laser confocal microscopy(Fig.1).

結果と考察 / Results and Discussion

Surfaces roughness maps were calculated by passing the surface height maps through a high-pass filter and a low-pass filter. The high-frequency components, in other word, the roughness was employed to characterize the out-of-plane deformation under sub-grain scale. By calculating the local variance maps, the slip bands can be revealed. The dwell-fatigue test was subsequently carried out after the surface characterization. Unfortunately, no cracks were observed within the area inspected. The relation between out-of-plane deformation along slip bands and the crack initiation remained unclear.

図・表・数式 / Figures, Tables and Equations


Fig.1 Local variance maps (left), and line profiles of local variance and F-values on a line crossing beta-colony, alpha-grain and grain boundary (right)


その他・特記事項(参考文献・謝辞等) / Remarks(References and Acknowledgements)


成果発表・成果利用 / Publication and Patents

論文・プロシーディング(DOIのあるもの) / DOI (Publication and Proceedings)
口頭発表、ポスター発表および、その他の論文 / Oral Presentations etc.
特許 / Patents

特許出願件数 / Number of Patent Applications:0件
特許登録件数 / Number of Registered Patents:0件

印刷する
PAGE TOP
スマートフォン用ページで見る